Which stainless grade: 316, 304 or 201?

Claim: grade selection should follow exposure. 316 for the harshest zone, 304 for normal indoor use, 201 not at all in coastal or humid projects.
Evidence: ASSDA's guidance refers to a selection tool recommending grades from 304 for urban or rural exposures up to duplex 2205 for severe marine, and to Australian practice where 304 or 316 is chosen depending on distance from the sea (ASSDA). On the 200 series, ASSDA states that the corrosion resistance of the newer chromium-manganese grades is generally inferior to similar chromium-nickel grades, that they are intended for milder environments, and that grade mix-ups have caused serious corrosion failures (ASSDA 200 series). A Euro Inox review adds that most early 200-series grades were under-alloyed for general and localised corrosion resistance.
| Exposure | Accessories and fittings | Comment |
|---|---|---|
| Seafront, sight of the sea, open windows, pool areas | SUS316 or brass with a quality finish | Shorter cleaning interval |
| Coastal town, air-conditioned, sheltered | SUS304 or brass | 316 for exposed balconies and outdoor showers |
| Inland, normal indoor bathroom | SUS304 or brass | Standard care |
| Any coastal or humid site | Not 201 or other 200-series | Write the exclusion on the PO |
The accessory ranges we source label each item's material: most series are listed in SS 304, at least one series is listed in SS316, others in brass or brass with stainless parts, and some items in zinc alloy with stainless parts. Ask for the material of each item, not of the "series". ASSDA also warns that magnetism has nothing to do with corrosion resistance, so a magnet test cannot tell 304 from 201; use a grade test or certificate. Our article on SUS304 vs SUS201 hardware covers the inspection side.
Brass or stainless for faucet and accessory bodies?

Claim: both work near the coast. What decides the outcome is that the finish protects the base metal, and that the base metal is still sound where the finish wears or is chipped.
Evidence: the faucet ranges we source list bodies in high-quality or low-lead copper alloy (brass) for most bathroom mixers and SUS304 for a group of kitchen faucets, with precision brushed and anti-fingerprint finishing on the stainless models. The accessory ranges we source describe a brass series built with welded joints, CNC machining and a thickened mounting base. Solid brass and stainless are both full-section metals: a scratch exposes more of the same metal rather than a different, weaker one.
| Body | Strength near the coast | Watch for |
|---|---|---|
| SUS316 | Highest resistance among common accessory grades | Surface finish and crevices still matter |
| SUS304 | Good indoors with cleaning | Pitting or staining where salt sits and is not cleaned |
| Brass, finished | Full-section metal under the coating | Finish quality; DZR where water contact applies |
| Zinc alloy, finished | Depends entirely on the coating | Avoid in exposed coastal rooms |
For water-contact parts, brass should also have dezincification resistance where the market requires it; see DZR brass evidence.
PVD or electroplating: which finish lasts near the sea?

Claim: choose the coating by evidence on the actual part, not by process name or salt-spray hours alone.
Evidence: the faucet ranges we source describe their coloured finishes as "PVD vacuum plating, precision brushed", while chrome is the standard plated finish. Any coating protects only as well as its weakest point: edges, threads, screw holes and areas the coating did not reach. Salt-spray hours are often quoted as proof, but ASTM B117 itself states that prediction of performance in natural environments has seldom been correlated with salt-spray results, and that correlation should only be considered where long-term atmospheric exposure supports it (ASTM B117-19).
- Ask what is under the colour: base metal, any underlayers, and how edges and holes are covered.
- Ask for a salt-spray report on the same item and finish, and read its scope and pass criteria.
- Approve a physical sample of each finish and keep it as the reference for later batches.
Background reading: what a PVD finish is and the limits of a salt-spray report.
Are zinc-alloy accessories acceptable on the coast?

Claim: keep zinc-alloy bodies out of exposed coastal rooms; use them only where a damaged coating would not matter or can be replaced easily.
Evidence: in the accessory ranges we source, several robe hooks, paper holders, towel bars and hook rails are listed as "Zinc Alloy + SS". Zinc alloy is not stainless: once the coating is chipped or worn at an edge, the alloy beneath is exposed directly to salt and moisture. Because the material is listed per item, it is easy to end up with mixed materials in one "set".
- Ask the supplier to mark the material of every line item on the quotation.
- For seafront rooms, replace zinc-alloy items with the SS304, SS316 or brass equivalent.
- Do not mix materials within a visible set unless the finish samples match.
What about screws, brackets and mixed metals?

Claim: a 316 towel rail held by plain steel screws fails at the screw. Fixings must match or be isolated.
Evidence: ASSDA lists three conditions for galvanic corrosion: the joint is wet with a conductive liquid, the metals are in contact, and their potentials are sufficiently different. A large noble area such as stainless coupled to a small active part concentrates the corrosion current on the small part. ASSDA recommends avoiding dissimilar pairs where contaminants are significant, or insulating them with plastic strips, washers or sleeves, and warns that paint is not a reliable insulator (ASSDA galvanic corrosion FAQ).
| Item | Specify |
|---|---|
| Wall screws for stainless accessories | Same grade as the accessory (316 with 316) |
| Brass accessories | Stainless screws with nylon washers or sleeves at the contact |
| Concealed mounting plates | Same material as the screws; drainage so water does not sit in the plate |
| Wall plugs | Plastic, not metal |
Do surface texture and design details matter?

Claim: smoother, more open shapes hold less salt and moisture and are easier to clean.
Evidence: for stainless steel, ASSDA cites a commonly used target of no more than 0.5 µm Ra for resistance to tea staining, notes that rough surfaces show significant staining, and says a mirror polish is the best mechanical finish for corrosion resistance (ASSDA). It also identifies crevices and places where runoff dries as higher-risk spots.
- Prefer polished or fine-brushed surfaces over coarse textures for the harshest zone.
- Knurled and deeply textured parts look good but trap residue; plan to clean them more often.
- Avoid shelves and trays that hold standing water; choose open or drained profiles.
- Check that wall flanges sit tight to the wall so moisture cannot collect behind them.
What cleaning routine keeps coastal hardware looking new?

Claim: regular fresh-water cleaning is the single most effective protection, and the wrong cleaner can cause the damage it is meant to prevent.
Evidence: ASSDA's rule of thumb is that if an adjacent window needs washing, the stainless steel needs washing too. It does not recommend domestic cleaners, even non-abrasive ones, because some contain chloride activators or bleach, and it cites a beachside council that washes exterior stainless every three to four months with low-chloride water and detergent followed by a fresh-water rinse (ASSDA). Inside a bathroom, the same logic applies at a shorter interval.
| Task | How | Starting interval |
|---|---|---|
| Wipe-down | Soft cloth, mild soap and fresh water; dry afterwards | Each housekeeping clean |
| Detail clean | Clean crevices, knurling, flanges and under shelves | Monthly; weekly for seafront rooms |
| Inspection | Look for brown staining, pitting, lifting finish, rust at screws | Quarterly |
| Avoid | Bleach, chloride-based or acidic cleaners, scouring pads | Always |
Put this table in the operator handover; see hotel fixture handover and care.
What should the specification and inspection say?

Copy-paste specification clause:
- All exposed stainless steel shall be SUS316 in rooms classified as seafront or poorly ventilated, and SUS304 minimum elsewhere. 200-series stainless steels shall not be used.
- Zinc-alloy bodies shall not be used in rooms classified as seafront.
- The material of each line item shall be stated on the quotation and packing list.
- Fixings shall be of the same stainless grade as the item, or isolated with non-metallic washers or sleeves where materials differ.
- Each finish shall be approved on a physical sample of the same item; any salt-spray report shall identify the item, finish and test standard.
- The supplier shall provide care instructions listing permitted and prohibited cleaning agents.
| Check | How |
|---|---|
| Grade | Grade test kit or certificate on a sample of stainless items |
| Material per item | Packing list against the approved material schedule |
| Finish | Compare with the approved sample under daylight |
| Coating edges | Inspect edges, holes and threads for bare spots |
| Fixings | Screw material matches the specification |
For the full arrival routine see receiving and inspecting fixtures on site.
Sources

Technical statements were checked against these sources in November 2026. Material data from our supply base is quoted from the accessory and faucet catalogs of the partner factories we work with.
- Australian Stainless Steel Development Association (ASSDA), Seven ways to prevent tea staining of stainless steel
- ASSDA, 200 series stainless steels (high manganese, CrMn)
- ASSDA, Technical FAQ: Galvanic / dissimilar metal corrosion
- Euro Inox, Austenitic Chromium-Manganese Stainless Steels – A European Approach (2012, PDF)
- ASTM International, ASTM B117-19 Standard Practice for Operating Salt Spray (Fog) Apparatus, Significance and Use
The zone guidance in this article is a buyer's rule of thumb built on these sources, not a corrosion warranty. For seafront or high-value projects, ask a corrosion specialist to assess the site.